Thermal deformation and solder of a BGA: TDM, X-ray and sections on an automotive board

Case studies

An electronic board deforms when it heats up, and its most sensitive component may deform differently from the board. How can this be measured during a reflow cycle, and how can we then check what it left behind in the solder? This is the question put to INSIDIX by an automotive supplier, using three complementary methods: TDM, X-ray radiography and metallographic sections.

The context: making the assembly of an onboard computer more reliable

In an automotive computer, BGA (Ball Grid Array) components are connected to the board by hundreds of solder balls. During reflow, the board and the component expand and bend at different rates. If the difference becomes too large, the balls can deform, crack or detach, with defects that sometimes appear only after months of use.

The supplier entrusted INSIDIX with three boards fitted with a BGA component. The objectives were threefold:

  • measure the deformation of the board and the BGA during a simulated reflow cycle;
  • compare the behaviour of the three samples;
  • check the quality of the solder joints by X-ray radiography and metallographic sections.

Three methods, one laboratory

  • TDM: full-field optical measurement of topography and deformation under a thermal profile. A 394 × 318 mm field for the whole board, a 48 × 38 mm field for the BGA alone, with a vertical resolution of ±3 µm on the board and ±1 µm on the component.
  • X-ray radiography: front and oblique views of the BGA before and after reflow, to detect short circuits, solder splashes and voids.
  • Metallographic sections: cutting, mounting and polishing, then optical microscope observation of the balls, intermetallics and the printed circuit board.
Electronic board installed in the thermal chamber of the TDM system

Electronic board installed in the thermal chamber of the TDM system, resting on graphite rods and instrumented with thermocouples.

Each board was heated according to a representative reflow profile, up to 240 °C, then cooled. Thermocouples placed on the board, including one right behind the BGA, controlled the thermal chamber and made it possible to link each measurement to its actual temperature.

TDM measurement: the board dishes, the component tilts

The board takes a bowl shape (concave) whose deflection reaches its maximum at around 130 to 150 °C, between −2.4 and −2.8 mm depending on the sample. It decreases near the solder solidification temperature (about 217 °C), and the behaviour repeats from one board to the next.

The BGA, for its part, is concave throughout the heating (from −13 to −28 µm) and then flips into a dome shape at 240 °C, with +24 to +31 µm. On the two components measured to the end of the cycle, the initial shape is not recovered on cooling.

Carte électronique en cycle de refusion : déformation en forme de bol mesurée par TDM à 130 °C

Electronic board

130 °C · deflection −2.8 mm (bowl shape, concave)
Composant BGA à 221 °C : déformation mesurée par TDM, encore concave

BGA component

221 °C · −16 µm (still concave)
Composant BGA à 240 °C : déformation mesurée par TDM, bascule en dôme

BGA component

240 °C · +31 µm (flips into a dome, convex)

TDM deformation maps of the board (130 °C) and of the BGA (221 °C then 240 °C): the component goes from concave to convex.

X-ray radiography: no shape defect, quantified voids

The radiographic images, taken before and after reflow from two angles, show no short circuit, no solder splash and no major deformation of the balls. An automatic void-rate calculation was carried out on several areas: it lies between 4 and 13% in the worst cases.

Radiographie X du BGA en vue de face : aucun court-circuit

Front view

no short circuit
Radiographie X du BGA en vue oblique : aucune projection de soudure

Oblique view

no solder splash
Détection automatique des voids dans les billes de soudure du BGA, taux de 4 à 13 %

Void rate

calculated automatically: 4 to 13%

X-ray radiograph of the BGA in front view and oblique view, then automatic void detection (in green) in the solder balls.

Metallographic sections: the diagnosis in the solder

A cutting plane was chosen on each of the three components, along the axis of maximum deformation revealed by TDM. The microscope observations complete what radiography does not distinguish:

  • slightly bowed BGAs, with 10 to 20 µm of deflection;
  • porosity in the balls, up to 100 µm in diameter;
  • intermetallic layers of 1 to 12 µm, with localised growth up to 148 µm;
  • a surface finish 3 to 8 µm thick;
  • cracks or brittleness on some balls;
  • on one of the components, a tilted copper pad under a corner ball and delamination of the printed circuit board prepreg.
Coupe métallographique d’une bille de soudure : croissance d’intermétalliques

Intermetallics

outgrowth up to 148 µm
Coupe métallographique d’une bille de soudure : porosités et inclusions

Porosity and inclusions

up to 100 µm in the ball
Coupe métallographique d’une bille de soudure : pad incliné et délamination du prépreg

Tilted pad

prepreg delamination

Sections of BGA solder balls: intermetallic growth, porosity and inclusions, tilted pad with prepreg delamination.

What the customer gets

A single report that links the measured deformation, the solder quality and the internal defects: deformation maps at each temperature step, signed values for board and component, radiographic images with void calculation, and annotated sections with measurements. Choosing the cutting plane from the TDM data avoids searching for the defect at random.

This type of study helps to qualify a reflow profile, compare boards or suppliers, or understand the origin of a defect observed in series. TDM is a measurement technology developed and patented by INSIDIX, presented on tdm-3d.org.

A similar need on your boards or components?

Board deformation, BGA solder reliability, failure analysis: discover our services for automotive and electronics, or contact us to describe your issue.